All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3110 57.69
Ferro Frit 3134 25.00
EPK Kaolin 7.19
Silica 10.12
Add Amount
Bentonite 2.02
Chrome Oxide 0.05
Red Iron Oxide 1.21
Soda Ash 2.02
Copper Carbonate 1.01
Cobalt Carbonate 4.30

Instructions


This glaze recipe originally came from a workshop with Lisa Orr.

This recipe was shared by Lorraine Olderman in the July/August 2019 issue of Pottery Making Illustrated.