All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 5.30
Titanium Dioxide 1.10
Zinc Oxide 26.30
Ferro Frit 3110 50.50
Silica 16.80
Add Amount
Cobalt Carbonate 0.50
Copper Carbonate 2.10
Manganese Dioxide 3.20

Instructions

Published in the July/August 2016 issue of Pottery Making Illustrated.

Crystalline glazes tend to run so test carefully and fire with a glaze catcher.
Crystalline glazes tend to run so test carefully and fire with a glaze catcher.