All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.87
(Nytal) Talc 14.02
Whiting 9.35
Zinc Oxide 9.35
Soda Feldspar 46.73
EPK Kaolin 18.68
Add Amount
Copper Carbonate 2.80

Instructions

Published in "Working Potter Glazes" in the June 2015 issue of Ceramics Monthly.

I apply this glaze by dipping into it. Shown here is Chameleon glaze layered over a thinned chun glaze pattern. Glaze goes dark when thicker and varied light green when thin. It can also go darker on porcelain.
Mix all ingredients together prior to adding the water.