All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 2.50
OM4 Ball Clay 1.00
Grolleg 3.00
EPK Kaolin 1.00
Silica (325 mesh) 2.50
Add Amount
Water 4.00
Darvan #7 20.00
Sodium Silicate 20.00
Mason Stain 6600 Black 15.00

Instructions

Published in "Lows-to-Mid-Range" by YunWook Mun, in the May 2014 issue of Ceramics Monthly.


I mix the water and the Darvan then add the dry ingredients. I add the stain last. The parts of the recipe are all in pounds.

It takes 5-10 minutes to cast depending on object's size and the dryness of the mold. This slip can be fired to cone 10 but after cone 6, the color is less intense.