All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 30.00
Albany/Alberta Slip 70.00
Add Amount
Black Iron Oxide 1.00
Mason Stain 6600 Black 15.00

Instructions

Published in "Glazes for Latex Resist" by Courtney Martin, in the Dec 2013 issue of Ceramics Monthly.
I fired these glazes to cone 10 in my wood kiln, and add 4-8 pounds of salt. When I've fired these glazes in friends' kilns, I've found that they also like hotter and saltier atmospheres. These are all very stable and I don't have any trouble with them running.

I add Epsom salts to each of these glazes. I like the way it helps keep the glaze in suspension, and I feel like it makes the glaze stronger after it is on the pot and before it's fired. Without the Epsom salts, I find the glaze to be dusty and hard to paint wax over.