All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 44.00
EPK Kaolin 11.00
Silica 45.00
Add Amount
Bentonite 2.00
Cobalt Carbonate 1.00

Instructions

Published in "Cone 02 Glaze Recipes" in the Feb 2015 issue of Ceramics Monthly.

Very runny low-fire glaze that forms crystals when cooled slowly. Not food safe.
Very runny! When applied thick, these are best fired on a horizontal surface. To achieve optimum crystal growth, slow cool the kiln at 90° per hour, from 1562° to 900°F. Not food safe.