All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Spodumene 13.00
Wollastonite 20.00
Zinc Oxide 8.00
Ferro Frit 3134 21.00
EPK Kaolin 20.00
Silica 18.00

Instructions

Published in "Keep It Hot, Hot, Hot" in the September/October 2015 issue of Pottery Making Illustrated.

The piece in the images shown here has the Campana Clear Base glaze over AMACO Velvet underglazes.
For different colors try adding copper carbonate, Praseodymium Yellow Mason stain, or Best Black Mason stain. Greens don't always work well with this base glaze, so always test first.