All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Spodumene 11.00
Wollastonite 20.00
Zinc 8.00
Ferro Frit 3134 21.00
Grolleg Kaolin 20.00
Silica 20.00
Add Amount
Bentonite 2.00

Instructions


Apply thinner; the glaze will drip when thick. Use a ball mill to help break down the zinc and sieve. I brush 3 layers for normal glazed areas and 4–6 coats where I want the glaze to run. Interacts well with colorants. (See page 46, image 1 for fired example.)

This recipe was shared by Jacob Monroe in the May 2021 issue of Ceramics Monthly.