All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 40.00
Whiting 10.00
Talc 5.00
EPK Kaolin 10.00
Borax 15.00
Silica 20.00
Add Amount
Rutile 10.00
Copper Carbonate 4.00

Instructions

Published in "Love the Frit You Have" by Deklan Ranlett, in the May/June 2013 issue of Pottery Making Illustrated.