All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 4.63
Ferro Frit 3124 9.26
Nepheline Syenite 24.07
EPK Kaolin 15.74
OM4 Ball Clay 23.15
Silica 23.15
Add Amount
Titanium Dioxide 9.26
Bentonite 1.85

Instructions

Shared by Brenda Lichman in "Soda Firing Slip & Glaze" in the Dec 2014 issue of Ceramics Monthly.

Image shown is porcelain, slip, Brenda's Titanium Butter, soda fired to cone 10.