All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 4.10
Minspar 200 Feldspar 18.40
Spodumene 15.40
Nepheline Syenite 45.50
OM 4 Ball Clay 16.60

Instructions

Published in "Atmospheric Glazes" by Lisa York, in the Dec 2015 issue of Ceramics Monthly. The image shown here was fired in reduction in a wood/soda kiln to cone 10.
Use hot water to dissolve soda ash when mixing to disperse the material and avoid clumping.