All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 20.20
Nepheline Syenite 3.03
OM 4 Ball Clay 27.27
Pyrophyllite 6.06
EPK Kaolin 27.28
Silica 16.16
Add Amount
Macaloid (Bentone MA) 1.01

Instructions


This recipe limits warping, and works very well when extruded, rolled, or pressed (it also throws like a dream). It fires to white with a yellow hue in oxidation, and white with a blue hue in reduction.

This recipe was shared by Forrest Lesch-Middelton in the October 2020 issue of Ceramics Monthly.