All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 22.70
Custer Feldspar 27.30
Grolleg Kaolin 19.10
Silica (325 Mesh) 30.90
Add Amount
Spanish Red Iron Oxide 0.40
Vanadium Blue Stain 1.40
Bentonite 1.00

Instructions

This recipe was shared by Alex Thullen in the January 2018 issue of Ceramics Monthly.
This glaze works well on textured surfaces. For the best color response, use over a white stoneware or porcelain clay body, or apply a white slip over darker clay bodies prior to bisque firing and glazing.