All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Water (in mL)* 800.00
Clay (Dry, in grams) 400.00
Deflocculant** 0.25

Instructions


*800 mL of water is 3 cups.

**For this batch size, use a few small drops of deflocculant.

This recipe yields about 500 grams of terra sigillata.

This recipe was shared by Rhonda Willers in the February 2021 issue of Ceramics Monthly, sourced from Terra Sigillata: Contemporary Techniques by Rhonda Willers.