All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 15.84
Ferro Frit 3134 9.90
Nepheline Syenite 21.29
EPK Kaolin 15.84
Silica 37.13
Add Amount
Red Iron Oxide 15.84

Instructions

Published in "Montana Glazes," in the Jan 2016 issue of Ceramics Monthly.

The piece in the image shown has multiple glazes on it including Black Persimmon (the darkest stripes).