All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 5.30
Talc 15.80
Ferro Frit 3124 15.80
OM 4 Ball Clay 15.80
Calcined Kaolin 21.00
EPK Kaolin 5.30
Silica 21.00
Add Amount
Zircopax 5.30

Instructions

Originally published in the Nov/Dec issue of Pottery Making Illustrated.

 
To mix the slip, measure each material, add to water, stir, and then sieve twice through a 60-mesh screen.