All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 65.80
Kona F-4 Feldspar 17.10
Nepheline Syenite 6.30
6 Tile Clay 10.80
Add Amount
Bentonite 2.00
Rutile 0.50
Zircopax 14.00

Instructions


Use less zircopax for a less-opaque-white liner glaze. I use only 10%.

Substitute Minspar 200 for the Kona F-4 feldspar.

This recipe was shared by Adero Willard in the September/October 2014 issue of Pottery Making Illustrated.