All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ball Clay 25.00
Cedar Heights Goldart 25.00
Hawthorne Bond (35 mesh) 25.00
Custer Feldspar 25.00

Instructions


This is a dependable, low-maintenance clay body that’s perfect for the classroom. It is especially good for stilts because its refractory character holds up in cone-14 wood firings with minimal structural issues. Roll coils at leather hard and stick the pins in before drying for 24 hours. Fire the stilts to cone 10 and you are good to go. Note: For other uses, substitute Hawthorne with EPK kaolin and you get a flashing porcelain. Substitute ball clay with Cedar Heights Redart and you get terra cotta.

This recipe was shared by Allen Chen in the March 2021 issue of Ceramics Monthly.