All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 6.37
Ball Clay 46.82
EPK Kaolin 46.81
Add Amount
Zircopax 11.73

Instructions


This is a flashing slip for the wood kiln.

After wadding the gallery, I place the lid on the pot and the whole piece on a bat. I spray a medium thickness of flashing slip evenly over the entire exterior. I let it dry on the bat until it is ready to load into the kiln. The soda vapors or wood ash create a glaze when they land on a piece during the firings, adding nuances of color and texture.

This recipe was shared Arlynn Nobel in the May/June 2021 issue of Pottery Making Illustrated.