All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 0.30
Whiting 33.40
Wood Ash 16.20
OM 4 Ball Clay 25.90
Silica (325 Mesh) 24.20
Add Amount
Cobalt 1.10
Red Iron Oxide 0.80
Rutile 4.30

Instructions


This glaze is a variation of others, and was developed further with my own experimentation. Wash, sieve, and dry the ash prior to adding it to the recipe. I use this glaze above Temple Black, which is applied to the lower section of the pot.

This recipe was shared by Seth Guzovsky in the January/February 2020 issue of Pottery Making Illustrated.