All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 4.50
Gerstley Borate 9.10
Ferro Frit 3110 31.90
Ball Clay 13.60
Kaolin 27.30
Silica 13.60

Instructions

This recipe was shared by Tom Bartel in the February 2019 issue of Ceramics Monthly.
This base is meant to be colored with commercial stains, not oxides.