All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 38.00
Custer Feldspar 52.00
EPK (Edgar Plastic Kaolin) 10.00
Add Amount
Mason Stain 6600 6.00

Instructions

Published in "Tom & Elaine Coleman" by John Nance, in the Jan 2003 issue of Ceramics Monthly