All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 6.80
Gerstley Borate 10.50
Talc 13.50
Whiting 9.00
Custer Feldspar 29.30
Kaolin 6.80
Silica 24.10
Add Amount
Zircopax 8.00

Instructions

Published in "School and Beyond" by Andy Cantrell, in the May 2000 issue of Ceramics Monthly.