All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3134 23.00
Ravenscrag Slip 75.00
Silica 2.00
Add Amount
Red Iron Oxide 8.00
Rutile 1.50

Instructions


I use this glaze often in my work and find that it's very reliable. It's a variation of Plainsman Clays' published come 6 Ravenscrag Clear glaze. For more color options, make tests that alter the percentages or types of colorants used.

This recipe was shared by Dawn Candy in the May 2019 issue of Ceramics Monthly.