All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 22.00
EPK Kaolin 28.00
OM4 Ball Clay 28.00
SIlica 22.00

Instructions

This recipe was shared in the January 2019 issue of Ceramics Monthly by Teresa Pietsch.
I mix up a large batch of white slip and pull out a cup at a time to mix with various colorants. I use 1/4  tsp to 2 tbsp of Mason stain, depending on my desired concentration.

This recipe works well in oxidation and reduction. I fire in an oxidation atmosphere with a slight body reduction between soda sprays at cone 03 and cone 01.