All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Strontium Carbonate 36.59
Nepheline Syenite 48.78
EPK Kaolin 2.43
Silica 12.20

Instructions


A simple strontium base, which can be colored with stains or oxides. A crater surface can be achieved with the addition of 2–5% magnesium carbonate. Shown with 5 and 10% titanium dioxide.

This recipe was shared by Alisa Liskin Clausen in the May 2019 issue of Ceramics Monthly.