All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 20.00
Ferro Frit 3134 20.00
Minspar 200 Feldspar 20.00
EPK Kaolin 20.00
Silica (325 Mesh) 20.00

Instructions


Mix to table cream consistency. This is a forgiving glaze with a wide working range of specific gravity and application thickness. It accepts Mason stains from 5–15%. Add 10% Mason stain 6236 Chartreuse for a bright green (see bowl interior).

This recipe was shared by Rita Vali in the January 2021 issue of Ceramics Monthly.