All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Water (in pounds)* 28.00
Clay (Dry, in pounds) 14.00
Add Amount
Deflocculant** 0.25

Instructions


*28 pounds of water is 3 1/2  gallons.

**For this batch size, use 1/4 cup of deflocculant.

This recipe yields about 2 gallons of terra sigillata.

This recipe was shared by Rhonda Willers in the February 2021 issue of Ceramics Monthly, sourced from Terra Sigillata: Contemporary Techniques by Rhonda Willers.