All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wood Ash 20.00
Ferro Frit 3134 20.00
Local Feldspar 20.00
EPK Kaolin 20.00
Silica 20.00

Instructions


When testing feldspars, try using Cuter Feldspar first. This glaze should be mixed very thin, to a specific gravity of 1.32.

This recipe was shared by Nathan Willever in the May 2019 issue of Ceramics Monthly.