Ingredients

Instructions

I mix this clear glaze recipe in 10,000-gram batches to fill a 5-gallon bucket. This glaze fires from cone 04–6, depending on clay type used. I fire to a hot cone 2, barely bending cone 3. This temperature works well for layering glazes to achieve the runny glaze drips I desire.

For Green add: 5–8% Copper Carbonate

For Light Brown add: 5–10% Iron Oxide

For Green Ocean Spray add: 8% Copper Carbonate and 8% Rutile

For Amber add: 5–10% Burnt Umber

For other glaze colors add: 5–20% stain

This recipe was shared by Nathan Bray in the September/October 2019 issue of Pottery Making Illustrated.

This item will be permanently deleted and cannot be recovered. Are you sure?

Once you submit this recipe for moderation you will no longer be able to edit its content.

Comments

Leave a Reply

You must be logged in to post a comment.

Enter Your Log In Credentials
This setting should only be used on your home or work computer.

Larger version of the image

Send this to a friend