Robbie’s Y altered

Robbie’s Y altered

Firing temperature : cone 8 | Surface texture : glossy | Color : cobalt blue | Atmosphere: Oxidation/Neutral

This glaze gives a nice gloss and holds colour well. I have altered Robbie's Y by substituting some of the ingredients that are more readily available to me.

The surface is lovely and glossy but not too glossy (could be more matt if fired lower). Drips are highly visible. Doesn't run and has the potential to grow interesting micro crystals on the surface so I will be doing some experimentation with firing for this.

 

Image shown with additions of cobalt carbonate 0.3, 0.5, 0.7, 0.9, 1.2 both brushed on and dipped.


Click Image to Enlarge

Ingredients

Instructions

-Needs to be sieved well

- fire to cone 8 with a 10 minute hold at the end

This item will be permanently deleted and cannot be recovered. Are you sure?

Once you submit this recipe for moderation you will no longer be able to edit its content.

Comments

Leave a Reply

You must be logged in to post a comment.

Enter Your Log In Credentials
This setting should only be used on your home or work computer.

Larger version of the image
Send this to a friend