All Purpose White Slip

Firing temperature : cone 04-10 | Surface texture : matte | Color : white | Atmosphere: Oxidation Reduction Soda

This recipe was shared in the January 2019 issue of Ceramics Monthly by Teresa Pietsch.


Click Image to Enlarge

Instructions

I mix up a large batch of white slip and pull out a cup at a time to mix with various colorants. I use 1/4  tsp to 2 tbsp of Mason stain, depending on my desired concentration.

This recipe works well in oxidation and reduction. I fire in an oxidation atmosphere with a slight body reduction between soda sprays at cone 03 and cone 01.

This item will be permanently deleted and cannot be recovered. Are you sure?

Once you submit this recipe for moderation you will no longer be able to edit its content.

Comments
  • thank you \ how much water do you add fot dipping, also what is your preferation to apply on leather hard or bone dry?

Leave a Reply

You must be logged in to post a comment.

Enter Your Log In Credentials
This setting should only be used on your home or work computer.

Larger version of the image

Send this to a friend